Procedure – Powder/Chip Samples
Determine the instrument blank.
Press the Analyze button on the instrument screen, the lower electrode will close and the analysis sequence will start and end automatically.
Repeat steps 2b through 2g a minimum of three times.
Set the blank following the procedure outlined in the operator's instruction manual.
Instrument calibration/drift correction.
Login a minimum of three Standard reps.
Weigh approximately *** grams of a calibration/drift standard into a *** Nickel Capsule; enter the mass and standard identification into appropriate rep fields. If applicable, place the nickel capsule in the appropriate autoloader position.
江苏LECO氧氮氢分析仪哪家好新型气路管道减少气路连接阀,使得漏气,断路故障更少。
736 Series: Oxygen/Nitrogen by Inert Gas Fusion
The 736 family of Elemental Analyzers is designed for routine measurement of oxygen and nitrogen content of
inorganic materials, ferrous and nonferrous alloys, andrefractory materials using the inert gas fusion technique.
These instruments feature our Cornerstone brand ® software, a custom interface designed specifically for
touch-screen operation. Developed by combining longterm research with customer feedback, this easy-to-use
software gives you complete access to instrument control, analysis settings, diagnostics, reporting, and more—without sacrificing valuable bench space.
ONH836氧氮氢分析仪
高频燃烧红外检测技分析无机材料中的碳、硫含量。
采用惰性气体保护熔融法,提供各种无机材料、钢铁、有色金属、硬质合金、难熔金属、陶瓷等材料中宽范围的氧氮氢同时分析。
该仪器配置MS Windows®的软件接口,专为触摸屏操作定制。长期的开发研究与客户反馈相结合,这个简单方便的软件使得用户可以快速完整访问仪器控制,分析设置,故障诊断,数据报告, **提高日常分析的效率并节省用户宝贵的时间。 可选的Cornerstone® Mobile软件功能,使得用户可以在手机,便携式电脑及台式电脑上便捷的访问仪器数据,分析曲线图形以及仪器的状态,实现对仪器的遥控。 分析软件同时包括实时的环境参数的监测,提供完整的系统图表的模拟。
Instrument calibration/drift correction.
a. Login a minimum of 3 Standard replicates.
b. Weigh a ~1.000 gram of a calibration/drift standard, enter the mass and standard identification into appropriate replicate fields.
c. Press the Analyze button on the instrument screen. After a short delay, the loading head slide-block will open.
d. Place the calibration/drift standard into the open port at the top of the loading head.
e. Press the Analyze button on the instrument screen again, the loading head slide-block will close and the lower electrode will open.
装有自动旁路阀的可快速拆装氧水捕集装置。安徽专业元素分析仪哪家好
力可**的动态流量补偿控制DFC系统,保证了流量系统的完善,可以精确控制整个气路中的流量。广东专业元素分析仪厂家供应
Procedure - Solid Samples:
--Instrument calibration/drift correction.
Place the nickel basket containing the calibration/drift standard into the open port at the top of the loading head.
Press the Analyze button on the instrument screen again, the loading head slide-block will close and the lower electrode will open.
Clean the upper and lower electrode manually, or, if applicable, remove the crucible and press the analyze button to clean with the automatic cleaner.
上海禹重实业有限公司是一家从事仪器科技、医疗科技、检测科技领域内的技术咨询、技术服务,仪器仪表的修理,仪器仪表、实验室设备、机械设备及配件、机电设备及配件、电子产品、化工产品及原料(除危险化学品、监控化学品、烟花爆竹、民用易爆物品、易制毒化学品)、第二类医疗器械的销售,机械设备租赁,电子商务,货物进出口,技术进出口。的公司,致力于发展为创新务实、诚实可信的企业。禹重科技拥有一支经验丰富、技术创新的专业研发团队,以高度的专注和执着为客户提供光谱仪,色谱仪,质谱仪,样品前处理。禹重科技继续坚定不移地走高质量发展道路,既要实现基本面稳定增长,又要聚焦关键领域,实现转型再突破。禹重科技始终关注仪器仪表市场,以敏锐的市场洞察力,实现与客户的成长共赢。
Procedure–Powder/ChipSamplesInstrumentcalibration/...
【详情】Procedure-SolidSamplesInstrumentcalibration/driftc
【详情】Procedure–Powder/ChipSamplesDeterminetheinstrument...
【详情】氧氮氢分析仪的常见故障及解决方法供电正常、通讯正常,点击确认键后分析仪不工作。这是没有水流,炉子温度...
【详情】Instrumentcalibration/driftcorrectionf.Cleantheupp
【详情】Procedure–Powder/ChipSamplesDeterminetheinstrument...
【详情】SamplePreparationTypically,titaniumandzirconiumsam
【详情】InstrumentHighlightsandFeaturesOptionalFeaturesOpt
【详情】